Qsmin test at 10 bar: the leak rate at 80 MPa is higher as at 60 MPa. This is not usual behaviour unless there is a change in gasket structure.
Gasket thickness at Qsmax sims to be very thin. Dont know how much the PTFE gasket can be destroyed.
I would suggest Pqr test at Qsmax and 250°C to evaluate if the gasket can withstand this parameters as long as necessary.
06-27-2024, 05:40 PM (This post was last modified: 06-27-2024, 05:41 PM by AVKO.)
+1 Agree here
(06-20-2024, 01:25 PM)Donit Wrote: Qsmin test at 10 bar: the leak rate at 80 MPa is higher as at 60 MPa. This is not usual behaviour unless there is a change in gasket structure.
Gasket thickness at Qsmax sims to be very thin. Dont know how much the PTFE gasket can be destroyed.
I would suggest Pqr test at Qsmax and 250°C to evaluate if the gasket can withstand this parameters as long as necessary.
07-15-2024, 01:19 PM (This post was last modified: 07-25-2024, 09:42 AM by AMTEC.)
Cross-check:
PQR @ 160MPa/250°C
The PQR value at 160 MPa/250 °C in the cross-check was 0,65 which is higher compared to the value of 0,63 which was submitted by the manufacturer. But the final thickness at the end of the test was below 0.1 mm, and the test sammple was damaged.
Therefore, we contatcetd the manufacturer and discussed the result. It turned out that uncorrected QSmax and PQR values were incorrectly transmitted when the data sheet was sent to amtec. At 100 °C and 250 °C, the maximum allowable gasket stresses were already significantly reduced. In the attachment you will find an updated evaluation of these corrected data.
We think, that the datasheet can be accepted in this form, and that a publication should be possible without any further cross-check.